Optical constants of HIKARI - PSK (Dense phosphate crown)
P-PSKH1S
Wavelength:
µm
(0.300 – 2.400)
Complex refractive index (n+ik)
n
k
LogX
LogY
eV
Derived optical constants
Dispersion formula
$$n^2=2.50002967-0.00669362188λ^{2}+0.0128441577λ^{-2}+0.000147794104λ^{-4}+2.25228249\text{×}10^{-06}λ^{-6}+5.14209979\text{×}10^{-08}λ^{-8}-5.44106184\text{×}10^{-05}λ^{4}$$Conditions & Spec sheet
n_absolute: false wavelength_vacuum: false temperature: 23.0 °C nd: 1.592550 Vd: 67.858832 glass_status: preferred density: 4.11 g/cm3 thermal_expansion: - temperature_range: -30 70 °C coefficient: 1.32e-05 K-1 dPgF: 0.0138
Comments
Low Tg glass
References
NIKON Zemax catalog 2017-11 (obtained from http://www.nikon.com)
See also HIKARI glass data sheets
Data
INFO
Hikari Glass Co., Ltd.
Hikari Glass Co., Ltd. is a Japanese glass maker, a subsidiary of Nikon Corp.External links
- Hikari Glass Co., Ltd. (in Japanese)
- Nikon