Optical constants of HIKARI - LaSF (Lanthanum dense flint)
E-LASFH9
Wavelength:
µm
(0.4 – 0.7)
Complex refractive index (n+ik)
n
k
LogX
LogY
eV
Derived optical constants
Dispersion formula
$$n^2=3.49989132-0.014925507λ^{2}+0.0384731987λ^{-2}+0.00184372906λ^{-4}-9.49882953\text{×}10^{-05}λ^{-6}+1.04373643\text{×}10^{-05}λ^{-8}$$Conditions & Spec sheet
n_absolute: false wavelength_vacuum: false temperature: 23.0 °C nd: 1.902650 Vd: 35.699754 glass_status: preferred density: 5.52 g/cm3 thermal_expansion: - temperature_range: -30 70 °C coefficient: 7.5e-06 K-1 dPgF: -0.0046
References
NIKON Zemax catalog 2017-11 (obtained from http://www.nikon.com)
See also HIKARI glass data sheets
Data
INFO
Hikari Glass Co., Ltd.
Hikari Glass Co., Ltd. is a Japanese glass maker, a subsidiary of Nikon Corp.External links
- Hikari Glass Co., Ltd. (in Japanese)
- Nikon