Optical constants of HIKARI - LaSF (Lanthanum dense flint)
E-LASFH6
Wavelength:
µm
(0.360 – 2.400)
Complex refractive index (n+ik)
n
k
LogX
LogY
eV
Derived optical constants
Dispersion formula
$$n^2=3.15292941-0.013157791λ^{2}+0.035267815λ^{-2}+0.00139578932λ^{-4}-3.80249631\text{×}10^{-05}λ^{-6}+9.59672806\text{×}10^{-06}λ^{-8}-8.30173359\text{×}10^{-05}λ^{4}$$Conditions & Spec sheet
n_absolute: false wavelength_vacuum: false temperature: 23.0 ℃ nd: 1.806100 Vd: 33.265207 glass_code: 806333 glass_status: preferred density: 3.76 g/cm3 thermal_expansion: - temperature_range: -30 70 ℃ coefficient: 8.3e-06 K-1 dPgF: 0.0025
References
NIKON Zemax catalog 2017-11 (obtained from http://www.nikon.com)
See also HIKARI glass data sheets
Data
INFO
Hikari Glass Co., Ltd.
Hikari Glass Co., Ltd. is a Japanese glass maker, a subsidiary of Nikon Corp.External links
- Hikari Glass Co., Ltd. (in Japanese)
- Nikon