Optical constants of HIKARI - LaK (Lanthanum crown)
LAK011
Wavelength:
µm
(0.290 – 0.7)
Complex refractive index (n+ik)
n
k
LogX
LogY
eV
Derived optical constants
Dispersion formula
$$n^2=2.971993-0.01524352λ^{2}+0.02020612λ^{-2}+0.0008752522λ^{-4}-7.671807\text{×}10^{-05}λ^{-6}+4.848072\text{×}10^{-06}λ^{-8}$$Conditions & Spec sheet
n_absolute: false wavelength_vacuum: false temperature: 20.0 °C nd: 1.741000 Vd: 52.672067 glass_code: 741527 glass_status: preferred density: 4.15 g/cm3 thermal_expansion: - temperature_range: -30 70 °C coefficient: 7e-06 K-1 dPgF: -0.01
References
NIKON Zemax catalog 2017-11 (obtained from http://www.nikon.com)
See also HIKARI glass data sheets
Data
INFO
Hikari Glass Co., Ltd.
Hikari Glass Co., Ltd. is a Japanese glass maker, a subsidiary of Nikon Corp.External links
- Hikari Glass Co., Ltd. (in Japanese)
- Nikon