Optical constants of HIKARI - LaK (Lanthanum crown)
J-LAK7
Wavelength:
µm
(0.280 – 2.400)
Complex refractive index (n+ik)
n
k
LogX
LogY
eV
Derived optical constants
Dispersion formula
$$n^2=2.6823272-0.0119713031λ^{2}-0.00014372436λ^{4}+0.0164555463λ^{-2}+0.000217295781λ^{-4}+4.69383509\text{×}10^{-06}λ^{-6}+3.49394854\text{×}10^{-08}λ^{-8}$$Conditions & Spec sheet
n_absolute: false wavelength_vacuum: false temperature: 23.0 ℃ thermal_dispersion: - type: "Schott formula" coefficients: -5.9728e-08 1.1901e-08 -5.8374e-13 5.2507e-07 5.712e-10 0.13665 nd: 1.651600 Vd: 58.571700 density: 3.3 g/cm3 thermal_expansion: - temperature_range: -30 70 ℃ coefficient: 6.6e-06 K-1 dPgF: -0.0045 phosphate_resistance: 4.0
References
NIKON Zemax catalog 2017-11 (obtained from http://www.nikon.com)
See also HIKARI glass data sheets