Optical constants of HIKARI - LaF (Lanthanum flint)
E-LAF04
Wavelength:
µm
(0.330 – 2.400)
Derived optical constants
n
k
logX
logY
eV
Dispersion formula
$$n^2=3.01654365-0.0142462083λ^{2}+0.0251223164λ^{-2}+0.000195992997λ^{-4}+4.35063641\text{×}10^{-05}λ^{-6}-7.85606637\text{×}10^{-07}λ^{-8}$$Conditions & Spec sheet
n_absolute: false wavelength_vacuum: false temperature: 23.0 °C nd: 1.756998 Vd: 47.826989 glass_code: 757478 glass_status: preferred density: 4.08 g/cm3 thermal_expansion: - temperature_range: -30 70 °C coefficient: 6.9e-06 K-1 dPgF: -0.0074
References
NIKON Zemax catalog 2017-11 (obtained from http://www.nikon.com)
See also HIKARI glass data sheets
Data
INFO
Hikari Glass Co., Ltd.
Hikari Glass Co., Ltd. is a Japanese glass maker, a subsidiary of Nikon Corp.External links
- Hikari Glass Co., Ltd. (in Japanese)
- Nikon