Optical constants of HIKARI - FK (Fluor crown)
E-FKH1
Wavelength:
µm
(0.290 – 2.400)
Complex refractive index (n+ik)
n
k
LogX
LogY
eV
Derived optical constants
Dispersion formula
$$n^2=2.22025427-0.00513496818λ^{2}+0.00841587708λ^{-2}+5.4263553\text{×}10^{-05}λ^{-4}+7.61288219\text{×}10^{-06}λ^{-6}-4.89857441\text{×}10^{-07}λ^{-8}$$Conditions & Spec sheet
n_absolute: false wavelength_vacuum: false temperature: 23.0 °C nd: 1.497820 Vd: 82.515656 glass_code: 498825 glass_status: preferred density: 3.87 g/cm3 thermal_expansion: - temperature_range: -30 70 °C coefficient: 1.53e-05 K-1 dPgF: 0.0331
References
NIKON Zemax catalog 2017-11 (obtained from http://www.nikon.com)
See also HIKARI glass data sheets