Optical constants of HIKARI - BaF (Barium flint)
E-BAF3
Wavelength:
µm
(0.350 – 2.400)
Complex refractive index (n+ik)
n
k
LogX
LogY
eV
Derived optical constants
Dispersion formula
$$n^2=2.43868193+0.00160996098λ^{2}+0.0268882943λ^{-2}-0.00244657917λ^{-4}+0.000396566086λ^{-6}-1.9730459\text{×}10^{-05}λ^{-8}$$Conditions & Spec sheet
n_absolute: false wavelength_vacuum: false temperature: 23.0 °C nd: 1.582670 Vd: 46.476921 glass_status: preferred density: 2.77 g/cm3 thermal_expansion: - temperature_range: -30 70 °C coefficient: 7.6e-06 K-1 dPgF: 0.0009
References
NIKON Zemax catalog 2017-11 (obtained from http://www.nikon.com)
See also HIKARI glass data sheets
Data
INFO
Hikari Glass Co., Ltd.
Hikari Glass Co., Ltd. is a Japanese glass maker, a subsidiary of Nikon Corp.External links