Optical constants of CDGM - ZPK (Dense phosphate crown)
H-ZPK7
Wavelength:
µm
(0.280 – 2.400)
Complex refractive index (n+ik)
n
k
LogX
LogY
eV
Derived optical constants
Dispersion formula
$$n^2-1=\frac{0.725400532λ^2}{λ^2-0.00296983783}+\frac{0.703767661λ^2}{λ^2-0.013434264}+\frac{0.77228314λ^2}{λ^2-135.211711}$$Conditions & Spec sheet
n_absolute: false wavelength_vacuum: false temperature: 20.0 ℃ thermal_dispersion: - type: "Schott formula" coefficients: -2.47e-05 -2.21e-09 5.2e-12 4.58e-07 5.69e-10 0.082 nd: 1.569070 Vd: 71.304254 glass_code: 569713 density: 4.36 g/cm3 thermal_expansion: - temperature_range: -30 70 ℃ coefficient: 1.34e-05 K-1 - temperature_range: 20 300 ℃ coefficient: 1.59e-05 K-1 dPgF: 0.02 climatic_resistance: 1.0
References
CDGM Zemax catalog 2022-06 (obtained from http://www.cdgmgd.com)
See also CDGM optical glass data sheets