Optical constants of CDGM - ZPK (Dense phosphate crown)
D-ZPK7-25
Wavelength:
µm
(0.280 – 2.400)
Complex refractive index (n+ik)
n
k
LogX
LogY
eV
Derived optical constants
Dispersion formula
$$n^2-1=\frac{0.71411271λ^2}{λ^2-0.0133604289}+\frac{0.713400795λ^2}{λ^2-0.0028939123}+\frac{0.765480668λ^2}{λ^2-134.125223}$$Conditions & Spec sheet
n_absolute: false wavelength_vacuum: false temperature: 20.0 ℃ thermal_dispersion: - type: "Schott formula" coefficients: -2.47e-05 -2.21e-09 5.2e-12 4.58e-07 5.69e-10 0.082 nd: 1.568540 Vd: 71.235367 glass_code: 569712 density: 4.36 g/cm3 thermal_expansion: - temperature_range: -30 70 ℃ coefficient: 1.33e-05 K-1 - temperature_range: 20 300 ℃ coefficient: 1.58e-05 K-1 dPgF: 0.0199 climatic_resistance: 1.0
Comments
anneal rate:25℃/h
References
CDGM Zemax catalog 2022-06 (obtained from http://www.cdgmgd.com)