Optical constants of CDGM - ZPK (Dense phosphate crown)
D-ZPK5-25
Wavelength:
µm
(0.280 – 2.400)
Complex refractive index (n+ik)
n
k
LogX
LogY
eV
Derived optical constants
Dispersion formula
$$n^2-1=\frac{0.353073711λ^2}{λ^2-0.0178712877}+\frac{1.14580426λ^2}{λ^2-0.00563723799}+\frac{0.795754681λ^2}{λ^2-125.202885}$$Conditions & Spec sheet
n_absolute: false wavelength_vacuum: false temperature: 20.0 ℃ thermal_dispersion: - type: "Schott formula" coefficients: -2.01e-05 4.05e-09 -1.52e-11 4e-07 1.43e-10 0.192 nd: 1.592160 Vd: 68.281511 glass_code: 592683 density: 4.29 g/cm3 thermal_expansion: - temperature_range: -30 70 ℃ coefficient: 1.23e-05 K-1 - temperature_range: 20 300 ℃ coefficient: 1.43e-05 K-1 dPgF: 0.0154 climatic_resistance: 1.0
Comments
anneal rate:25℃/h
References
CDGM Zemax catalog 2022-06 (obtained from http://www.cdgmgd.com)
See also CDGM optical glass data sheets