Optical constants of CDGM - ZLAF (Dense lanthanum flint)
H-ZLAF89L
Wavelength:
µm
(0.360 – 2.400)
Complex refractive index (n+ik)
n
k
LogX
LogY
eV
Derived optical constants
Dispersion formula
$$n^2=3.66932806-0.0136919991λ^{2}+0.0484216361λ^{-2}+0.00132160482λ^{-4}+2.4217258\text{×}10^{-05}λ^{-6}+8.50124351\text{×}10^{-06}λ^{-8}$$Conditions & Spec sheet
n_absolute: false wavelength_vacuum: false temperature: 20.0 °C thermal_dispersion: - type: "Schott formula" coefficients: -4.45e-07 1.4e-08 -3.45e-11 9.44e-07 1.04e-09 0.253 nd: 1.953749 Vd: 32.318108 glass_code: 954323 density: 5.1 g/cm3 thermal_expansion: - temperature_range: -30 70 °C coefficient: 7.2e-06 K-1 - temperature_range: 20 300 °C coefficient: 8.8e-06 K-1 dPgF: -0.0002 climatic_resistance: 1.0
References
CDGM Zemax catalog 2017-09 (obtained from http://www.cdgmgd.com)