Optical constants of CDGM - ZLAF (Dense lanthanum flint)
H-ZLAF53B
Wavelength:
µm
(0.350 – 2.400)
Complex refractive index (n+ik)
n
k
LogX
LogY
eV
Derived optical constants
Dispersion formula
$$n^2=3.25780649-0.0123377843λ^{2}+0.0355171622λ^{-2}+0.000705690228λ^{-4}+4.3498733\text{×}10^{-05}λ^{-6}+1.95613611\text{×}10^{-06}λ^{-8}$$Conditions & Spec sheet
n_absolute: false wavelength_vacuum: false temperature: 20.0 °C thermal_dispersion: - type: "Schott formula" coefficients: 9.9e-06 2.08e-08 -8.84e-11 8.92e-07 6.66e-10 0.24 nd: 1.833996 Vd: 37.229136 glass_code: 834372 glass_status: standard density: 4.54 g/cm3 thermal_expansion: - temperature_range: -30 70 °C coefficient: 5.9e-06 K-1 - temperature_range: 20 300 °C coefficient: 7.2e-06 K-1 dPgF: -0.0041 climatic_resistance: 1.0
References
CDGM Zemax catalog 2017-09 (obtained from http://www.cdgmgd.com)