Optical constants of CDGM - ZLAF (Dense lanthanum flint)
D-ZLAF81-25
Wavelength:
µm
(0.340 – 2.400)
Complex refractive index (n+ik)
n
k
LogX
LogY
eV
Derived optical constants
Dispersion formula
$$n^2-1=\frac{1.90958888λ^2}{λ^2-0.0102182926}+\frac{0.266893034λ^2}{λ^2-0.0421328894}+\frac{1.26585975λ^2}{λ^2-97.0733228}$$Conditions & Spec sheet
n_absolute: false wavelength_vacuum: false temperature: 20.0 ℃ thermal_dispersion: - type: "Schott formula" coefficients: 5.18e-06 1.52e-08 1.59e-10 5.99e-07 9.97e-11 0.282 nd: 1.807570 Vd: 40.973340 glass_code: 808410 density: 4.55 g/cm3 thermal_expansion: - temperature_range: -30 70 ℃ coefficient: 6.4e-06 K-1 - temperature_range: 20 300 ℃ coefficient: 8.1e-06 K-1 dPgF: -0.006
Comments
anneal rate:25℃/h
References
CDGM Zemax catalog 2022-06 (obtained from http://www.cdgmgd.com)