Optical constants of CDGM - ZLAF (Dense lanthanum flint)
D-ZLAF67-25
Wavelength:
µm
(0.350 – 2.400)
Complex refractive index (n+ik)
n
k
LogX
LogY
eV
Derived optical constants
Dispersion formula
$$n^2-1=\frac{1.36012388λ^2}{λ^2-103.579888}+\frac{2.09601012λ^2}{λ^2-0.011037962}+\frac{0.333537105λ^2}{λ^2-0.0449413554}$$Conditions & Spec sheet
n_absolute: false wavelength_vacuum: false temperature: 20.0 ℃ thermal_dispersion: - type: "Schott formula" coefficients: 3.22e-06 1.64e-08 -4.25e-11 8.62e-07 7.87e-10 0.235 nd: 1.882590 Vd: 37.185491 glass_code: 883372 density: 5.5 g/cm3 thermal_expansion: - temperature_range: -30 70 ℃ coefficient: 6.7e-06 K-1 - temperature_range: 20 300 ℃ coefficient: 8.5e-06 K-1 dPgF: -0.0047 climatic_resistance: 1.0
Comments
anneal rate:25℃/h
References
CDGM Zemax catalog 2022-06 (obtained from http://www.cdgmgd.com)