Optical constants of CDGM - ZK (Dense crown)
H-ZK50
Wavelength:
µm
(0.290 – 2.400)
Complex refractive index (n+ik)
n
k
LogX
LogY
eV
Derived optical constants
Dispersion formula
$$n^2-1=\frac{0.434311306λ^2}{λ^2+0.00192252587}+\frac{1.10560033λ^2}{λ^2-0.0147271072}+\frac{0.988776159λ^2}{λ^2-110.41165}$$Conditions & Spec sheet
n_absolute: false wavelength_vacuum: false temperature: 20.0 ℃ thermal_dispersion: - type: "Schott formula" coefficients: 3.24e-06 1.77e-08 -2.57e-11 5.34e-07 1.22e-10 0.194 nd: 1.607380 Vd: 56.654511 glass_code: 607567 density: 3.54 g/cm3 thermal_expansion: - temperature_range: -30 70 ℃ coefficient: 6.8e-06 K-1 - temperature_range: 20 300 ℃ coefficient: 7.7e-06 K-1 dPgF: -0.001 climatic_resistance: 1.0
References
CDGM Zemax catalog 2022-06 (obtained from http://www.cdgmgd.com)
See also CDGM optical glass data sheets