Optical constants of CDGM - ZK (Dense crown)
H-ZK14
Wavelength:
µm
(0.290 – 2.400)
Complex refractive index (n+ik)
n
k
LogX
LogY
eV
Derived optical constants
Dispersion formula
$$n^2-1=\frac{0.821911395λ^2}{λ^2-0.00369659724}+\frac{0.995367381λ^2}{λ^2-97.9765358}+\frac{0.708381156λ^2}{λ^2-0.0159409871}$$Conditions & Spec sheet
n_absolute: false wavelength_vacuum: false temperature: 20.0 ℃ thermal_dispersion: - type: "Schott formula" coefficients: 3.66e-07 1.7e-08 -3.14e-11 3.59e-07 3.53e-10 0.219 nd: 1.603110 Vd: 60.603787 glass_code: 603606 glass_status: standard density: 3.44 g/cm3 thermal_expansion: - temperature_range: -30 70 ℃ coefficient: 6.1e-06 K-1 - temperature_range: 20 300 ℃ coefficient: 7.5e-06 K-1 dPgF: -0.0011
References
CDGM Zemax catalog 2022-06 (obtained from http://www.cdgmgd.com)