Optical constants of CDGM - ZK (Dense crown)
D-ZK3-25
Wavelength:
µm
(0.290 – 2.400)
Complex refractive index (n+ik)
n
k
LogX
LogY
eV
Derived optical constants
Dispersion formula
$$n^2-1=\frac{1.24347604λ^2}{λ^2-108.031442}+\frac{0.918798491λ^2}{λ^2-0.0139520404}+\frac{0.567180042λ^2}{λ^2-0.00127620015}$$Conditions & Spec sheet
n_absolute: false wavelength_vacuum: false temperature: 20.0 ℃ thermal_dispersion: - type: "Schott formula" coefficients: 1.68e-06 9.68e-09 -2e-11 5.34e-07 1.41e-09 0.172 nd: 1.588330 Vd: 61.284362 glass_code: 588613 density: 2.83 g/cm3 thermal_expansion: - temperature_range: -30 70 ℃ coefficient: 7.2e-06 K-1 - temperature_range: 20 300 ℃ coefficient: 9.3e-06 K-1 dPgF: -0.0039 climatic_resistance: 4.0
Comments
anneal rate:25℃/h
References
CDGM Zemax catalog 2022-06 (obtained from http://www.cdgmgd.com)