Optical constants of CDGM - ZK (Dense crown)
D-ZK3
Wavelength:
µm
(0.290 – 2.400)
Complex refractive index (n+ik)
n
k
LogX
LogY
eV
Derived optical constants
Dispersion formula
$$n^2=2.48968705-0.0121700502λ^{2}+0.0125749866λ^{-2}+0.000532456449λ^{-4}-5.1039362\text{×}10^{-05}λ^{-6}+2.86502873\text{×}10^{-06}λ^{-8}$$Conditions & Spec sheet
n_absolute: false wavelength_vacuum: false temperature: 20.0 °C thermal_dispersion: - type: "Schott formula" coefficients: 1.68e-06 9.68e-09 -2e-11 5.34e-07 1.41e-09 0.172 nd: 1.589132 Vd: 61.162960 glass_code: 589612 density: 2.83 g/cm3 thermal_expansion: - temperature_range: -30 70 °C coefficient: 7.2e-06 K-1 - temperature_range: 20 300 °C coefficient: 9.3e-06 K-1 dPgF: -0.007 climatic_resistance: 4.0
References
CDGM Zemax catalog 2017-09 (obtained from http://www.cdgmgd.com)