Optical constants of CDGM - ZK (Dense crown)
D-ZK2L-25
Wavelength:
µm
(0.300 – 2.400)
Complex refractive index (n+ik)
n
k
LogX
LogY
eV
Derived optical constants
Dispersion formula
$$n^2-1=\frac{0.530248488λ^2}{λ^2-0.0175027403}+\frac{1.12537335λ^2}{λ^2-109.192004}+\frac{0.947317341λ^2}{λ^2-0.00498306497}$$Conditions & Spec sheet
n_absolute: false wavelength_vacuum: false temperature: 20.0 ℃ thermal_dispersion: - type: "Schott formula" coefficients: 2.09e-06 1.37e-08 -3.16e-11 4.84e-07 4.03e-10 0.189 nd: 1.586250 Vd: 59.524868 glass_code: 586595 density: 2.99 g/cm3 thermal_expansion: - temperature_range: 20 300 ℃ coefficient: 9e-06 K-1 dPgF: -0.0035
Comments
anneal rate:25℃/h
References
CDGM Zemax catalog 2022-06 (obtained from http://www.cdgmgd.com)
See also CDGM optical glass data sheets