Optical constants of CDGM - ZF (Dense flint)
H-ZF3
Wavelength:
µm
(0.360 – 2.400)
Complex refractive index (n+ik)
n
k
LogX
LogY
eV
Derived optical constants
Dispersion formula
$$n^2-1=\frac{0.203624748λ^2}{λ^2-0.0620712732}+\frac{1.64202576λ^2}{λ^2-0.0127139992}+\frac{1.38768085λ^2}{λ^2-128.254467}$$Conditions & Spec sheet
n_absolute: false wavelength_vacuum: false temperature: 20.0 ℃ thermal_dispersion: - type: "Schott formula" coefficients: -4.82e-06 1.32e-08 -3.85e-11 9.08e-07 1.03e-09 0.282 nd: 1.717360 Vd: 29.499110 glass_code: 717295 glass_status: standard density: 3.06 g/cm3 thermal_expansion: - temperature_range: -30 70 ℃ coefficient: 9e-06 K-1 - temperature_range: 20 300 ℃ coefficient: 1.12e-05 K-1 dPgF: 0.0093 climatic_resistance: 1.0
References
CDGM Zemax catalog 2022-06 (obtained from http://www.cdgmgd.com)
See also CDGM optical glass data sheets