$$n^2=3.05150937-0.0123177102λ^{2}+0.0421532614λ^{-2}+0.00181669625λ^{-4}-2.87661517\text{×}10^{-05}λ^{-6}+1.88518506\text{×}10^{-05}λ^{-8}$$Conditions & Spec sheet
n_absolute: false wavelength_vacuum: false temperature: 20.0 °C thermal_dispersion: - type: "Schott formula" coefficients: -4.97e-06 1.25e-08 2.17e-11 1.02e-06 2.47e-09 0.282 nd: 1.784721 Vd: 25.719658 glass_code: 785257 glass_status: standard density: 3.25 g/cm3 thermal_expansion: - temperature_range: -30 70 °C coefficient: 8.6e-06 K-1 - temperature_range: 20 300 °C coefficient: 1.06e-05 K-1 dPgF: 0.0149 climatic_resistance: 1.0
References
CDGM Zemax catalog 2017-09 (obtained from http://www.cdgmgd.com)