Optical constants of CDGM - LAK (Lanthanum crown)
D-LAK6-25
Wavelength:
µm
(0.300 – 2.400)
Complex refractive index (n+ik)
n
k
LogX
LogY
eV
Derived optical constants
Dispersion formula
$$n^2-1=\frac{1.22299893λ^2}{λ^2-94.0859262}+\frac{0.471209941λ^2}{λ^2-0.0227830104}+\frac{1.33928922λ^2}{λ^2-0.00665285316}$$Conditions & Spec sheet
n_absolute: false wavelength_vacuum: false temperature: 20.0 ℃ thermal_dispersion: - type: "Schott formula" coefficients: 1.33e-06 1.27e-08 -2.36e-11 5.62e-07 7.08e-10 0.199 nd: 1.692810 Vd: 53.049215 glass_code: 693531 density: 3.5 g/cm3 thermal_expansion: - temperature_range: -30 70 ℃ coefficient: 7.5e-06 K-1 - temperature_range: 20 300 ℃ coefficient: 9.5e-06 K-1 dPgF: -0.0083 climatic_resistance: 1.0
Comments
anneal rate:25℃/h
References
CDGM Zemax catalog 2022-06 (obtained from http://www.cdgmgd.com)
See also CDGM optical glass data sheets