Optical constants of CDGM - FK (Fluor crown)
H-FK71A
Wavelength:
µm
(0.280 – 2.400)
Complex refractive index (n+ik)
n
k
LogX
LogY
eV
Derived optical constants
Dispersion formula
$$n^2=2.1034791-0.0050373404λ^{2}+0.00629672175λ^{-2}+0.000223232867λ^{-4}-2.25577913\text{×}10^{-05}λ^{-6}+1.15904431\text{×}10^{-06}λ^{-8}$$Conditions & Spec sheet
n_absolute: false wavelength_vacuum: false temperature: 20.0 ℃ thermal_dispersion: - type: "Schott formula" coefficients: -2.19e-05 -1.02e-08 -3.61e-11 4.81e-07 1.36e-09 0.08 nd: 1.456498 Vd: 90.470884 glass_code: 457905 glass_status: preferred density: 3.64 g/cm3 thermal_expansion: - temperature_range: -30 70 ℃ coefficient: 1.36e-05 K-1 - temperature_range: 20 300 ℃ coefficient: 1.74e-05 K-1 dPgF: 0.0415 climatic_resistance: 1.0
References
CDGM Zemax catalog 2022-06 (obtained from http://www.cdgmgd.com)
See also CDGM optical glass data sheets