Optical constants of CDGM - FK (Fluor crown)
H-FK61
Wavelength:
µm
(0.290 – 2.400)
Complex refractive index (n+ik)
n
k
LogX
LogY
eV
Derived optical constants
Dispersion formula
$$n^2=2.21667349-0.00493991656λ^{2}+0.00915004725λ^{-2}-0.00012667557λ^{-4}+2.8243403\text{×}10^{-05}λ^{-6}-1.31517813\text{×}10^{-06}λ^{-8}$$Conditions & Spec sheet
n_absolute: false wavelength_vacuum: false temperature: 20.0 °C thermal_dispersion: - type: "Schott formula" coefficients: -2.02e-05 3.72e-09 -1.25e-11 2.98e-07 -1.9e-10 0.228 nd: 1.496998 Vd: 81.594687 glass_code: 497816 glass_status: standard density: 3.7 g/cm3 thermal_expansion: - temperature_range: -30 70 °C coefficient: 1.31e-05 K-1 - temperature_range: 20 300 °C coefficient: 1.57e-05 K-1 dPgF: 0.0286 climatic_resistance: 1.0
References
CDGM Zemax catalog 2017-09 (obtained from http://www.cdgmgd.com)