Optical constants of CDGM - FK (Fluor crown)
D-FK61A
Wavelength:
µm
(0.290 – 2.400)
Complex refractive index (n+ik)
n
k
LogX
LogY
eV
Derived optical constants
Dispersion formula
$$n^2-1=\frac{0.714812161λ^2}{λ^2-0.0108370689}+\frac{0.502984998λ^2}{λ^2-0.00132155859}+\frac{0.836119846λ^2}{λ^2-153.360674}$$Conditions & Spec sheet
n_absolute: false wavelength_vacuum: false temperature: 20.0 ℃ thermal_dispersion: - type: "Schott formula" coefficients: -1.94e-05 2.54e-09 -2.83e-11 3.05e-07 -9.31e-11 0.242 nd: 1.497000 Vd: 81.605419 glass_code: 497816 glass_status: standard density: 3.68 g/cm3 thermal_expansion: - temperature_range: -30 70 ℃ coefficient: 1.26e-05 K-1 - temperature_range: 20 300 ℃ coefficient: 1.55e-05 K-1 dPgF: 0.031 climatic_resistance: 1.0
Comments
anneal rate:4℃/h
References
CDGM Zemax catalog 2022-06 (obtained from http://www.cdgmgd.com)
See also CDGM optical glass data sheets