Dispersion formula
$$n^2-1=\frac{0.894432499λ^2}{λ^2-0.00436678978}+\frac{0.321652123λ^2}{λ^2-0.0141909741}+\frac{0.748704285λ^2}{λ^2-149.771388}$$Conditions & Spec sheet
n_absolute: false wavelength_vacuum: false temperature: 20.0 ℃ thermal_dispersion: - type: "Schott formula" coefficients: -2.45e-05 -2.09e-09 -6.72e-13 3.69e-07 2.37e-10 0.173 nd: 1.496530 Vd: 81.531772 glass_code: 497815 density: 3.9 g/cm3 thermal_expansion: - temperature_range: -30 70 ℃ coefficient: 1.45e-05 K-1 - temperature_range: 20 300 ℃ coefficient: 1.7e-05 K-1 dPgF: 0.0321 climatic_resistance: 1.0
Comments
anneal rate:25℃/h
References
CDGM Zemax catalog 2022-06 (obtained from http://www.cdgmgd.com)