Optical constants of CDGM - F (Flint)
H-F5

Wavelength: µm
 (0.360 – 2.400)  
 

Complex refractive index (n+ik)[ i ]


n   k   LogX   LogY   eV

Derived optical constants

Dispersion formula [ i ]

$$n^2-1=\frac{1.43541709λ^2}{λ^2-0.0108394789}+\frac{0.133104631λ^2}{λ^2-0.058152846}+\frac{1.2215186λ^2}{λ^2-120.768299}$$

Conditions & Spec sheet

n_absolute: false
wavelength_vacuum: false
temperature: 20.0 ℃
thermal_dispersion:
  - type: "Schott formula"
    coefficients: -7.35e-07 1.37e-08 -1.86e-11 7.71e-07 6.53e-10 0.265
nd: 1.624350
Vd: 35.923444
glass_code: 624359
density: 2.69 g/cm3
thermal_expansion:
  - temperature_range: -30 70 ℃
    coefficient: 7.8e-06 K-1
  - temperature_range: 20 300 ℃
    coefficient: 9.7e-06 K-1
dPgF: 0.0046
climatic_resistance: 1.0

References

CDGM Zemax catalog 2022-06 (obtained from http://www.cdgmgd.com)
See also CDGM optical glass data sheets

Data

[Expressions for n]   [CSV - comma separated]   [TXT - tab separated]   [Full database record]

INFO

CDGM Glass Co., Ltd.

CDGM Glass Co., Ltd. is a leading optical glass supplier in China with a worldwile distribution network.

External links


Glass

External links