Optical constants of (C5H8O2)n (Poly(methyl methacrylate), PMMA)
Beadie et al. 2015: n 0.42–1.62 µm
Complex refractive index (n+ik)
Derived optical constants
Dispersion formula
$$n^2=2.1778+6.1209\text{×}10^{-3}λ^{2}-1.5004\text{×}10^{-3}λ^{4}+2.3678\text{×}10^{-2}λ^{-2}-4.2137\text{×}10^{-3}λ^{-4}+7.3417\text{×}10^{-4}λ^{-6}-4.5042\text{×}10^{-5}λ^{-8}$$Conditions
temperature: 293.25
Notes
20.1 °C. Absolute accuracy < 2×10-4.
References
G. Beadie, M. Brindza, R. A. Flynn, A. Rosenberg, J. S. Shirk. Refractive index measurements of poly(methyl methacrylate) (PMMA) from 0.4-1.6 μm. Appl. Opt. 54, F139-F143 (2015)
Data
Additional information
About Poly(methyl methacrylate)
Pentanol (Amyl alcohol, C5H12O) is an organic compound that belongs to the alcohol family. There are several isomers of pentanol, with the common name "amyl alcohol" often referring to a mixture of these isomers. Predominantly, it's used as a solvent and an intermediate in the production of other chemicals. In its pure form, pentanol has a characteristic alcoholic odor and is slightly viscous compared to lower alcohols. When considering its optical properties, pentanol is generally transparent in the visible spectrum. Like other alcohols, pentanol should be handled with care due to its flammable nature and potential health effects. Proper storage and precautions are necessary when working with or around this compound.
Other names and variations
- (C5H8O2)n
- Poly(methyl methacrylate)
- PMMA
- Acrylic glass
- Plexiglas
- Vitroflex
- Limacryl
- R-Cast
- Per-Clax
- Perspex
- Plazcryl
- Acrylex
- Acrylite
- Acrylplast
- Altuglas
- Polycast
- Oroglass
- Lucite
Links