Optical constants of Fused silica (fused quartz)
Malitson 1965: n 0.21–3.71 µm
Complex refractive index (n+ik)
Derived optical constants
Dispersion formula
$$n^2-1=\frac{0.6961663λ^2}{λ^2-0.0684043^2}+\frac{0.4079426λ^2}{λ^2-0.1162414^2}+\frac{0.8974794λ^2}{λ^2-9.896161^2}$$Conditions
temperature: 293
Comments
Fused silica, 20 °C
References
- I. H. Malitson.
Interspecimen comparison of the refractive index of fused silica.
J. Opt. Soc. Am. 55, 1205-1208 (1965)
- C. Z. Tan.
Determination of refractive index of silica glass for infrared wavelengths by IR spectroscopy.
J. Non-Cryst. Solids 223, 158-163 (1998)
- Sellmeier formula is reported in Ref. 1 for the 0.21–3.71 μm wavelength range. Ref. 2 verifies the validity of the formula up to 6.7 μm.
Data
Additional information
About Silicon dioxide
Silicon dioxide (SiO2), commonly known as silica, is found naturally in several crystalline forms, the most notable being quartz. Additionally, when silicon dioxide is manufactured without the crystalline structure, it forms what is known as fused silica. Fused silica is a non-crystalline (or amorphous) form of silicon dioxide and is produced by melting high purity silica at extremely high temperatures. It has superior optical clarity, especially in the ultraviolet (UV) range, and is resistant to thermal shock, making it valuable for many high-end optical applications, including lenses and windows in spacecraft and satellites. SiO2 is extensively used in electronics as an insulator and serves as a primary ingredient in the production of glass. It's also used in thin-film optics, often as antireflection coatings on optical devices. Beyond its optical applications, silicon dioxide finds use in ceramics, construction, and even as a food additive.
Polymorphs
- Alpha quartz (α-quartz, most common)
- Beta quartz (β-quartz, only stable at temperatures above 573 °C)
- Tridymite
- Cristobalite
- Coesite
- Stishovite
- Lechatelierite
- Chalcedony
Other names and variations
- SiO2
- Quartz
- Silica
- Silicon oxide
- Silicon(IV) dioxide
Links