Optical constants of SrF2 (Strontium fluoride)
Feldman et al. 1978: n 0.21–11.5 µm
Complex refractive index (n+ik)
Derived optical constants
Dispersion formula
$$n^2-1=\frac{0.67805894λ^2}{λ^2-0.05628989^2}+\frac{0.37140533λ^2}{λ^2-0.10801027^2}+\frac{3.3485284λ^2}{λ^2-39.906666^2}$$Comments
20 °C
References
A. Feldman, D. Horowitz, R. Waxier and M. Dodge. [Optical materials characterization final technical report, February 1, 1978.](https://refractiveindex.info/download/data/1978/Feldman 1978 - Optical materials characterization final technical report.pdf)
Data
Additional information
About Strontium fluoride
Strontium fluoride (SrF2) is an inorganic compound that appears as a white crystalline solid at room temperature. With a high melting point and good thermal stability, it is often used in optical applications due to its notable transparency to ultraviolet and visible wavelengths. Its optical clarity has led to its use in the manufacture of windows and lenses, especially in specialized optical systems. Additionally, SrF2 is employed as a thin film in the production of optical coatings, thanks to its low refractive index. Moreover, the compound is explored for potential use in fluoride ion batteries due to its high ionic conductivity. In nature, strontium fluoride occurs as the mineral strontianite, though most commercial preparations are synthesized through chemical reactions.
Other names and variations
- SrF2
- Strontium difluoride
- Strontium(II) fluoride
Links