Optical constants of SUMITA - Optical glass
K-PSFn1(M)

Wavelength: µm
 (0.380–2.000)  
 

Complex refractive index (n+ik)[ i ]


n   k   LogX   LogY   eV

Derived optical constants

Dispersion formula

$$n^2=3.418365-0.015830577λ^{2}+0.056024892λ^{-2}+0.0042907055λ^{-4}-0.00027089374λ^{-6}+4.8560287\text{×}10^{-05}λ^{-8}$$

Conditions

temperature: 293

References

Data

[Expressions for n]   [CSV - comma separated]   [TXT - tab separated]   [Full database record]

Additional information

Properties of K-PSFn1(M)

thermal_dispersion:
  - 
    type: formula A
    coefficients: -3.11e-06 1.75e-08 -2.81e-10 1.25e-06 1.62e-09 0.307
nd: 1.89945
Vd: 21.3
glass_code: 907212
density:
  - 
    value: 4150
thermal_expansion:
  - 
    temperature_range: 243 343
    value: 7.4E-6
  - 
    temperature_range: 293 573
    value: 1.02E-5
dPgF: 0.0238
resistance:
  climatic: "1.0"
  acid: "1.0"

About

SUMITA Optical Glass, Inc. is a Japanese corporation known for its specialization in the production and development of optical glass, optical fiber, and various other photonic products. Founded in 1953, the company has established itself as a leading provider of high-quality optical materials that are used in a wide range of applications—from industrial and scientific optics to consumer electronics and medical devices. SUMITA's portfolio includes a variety of specialized optical glasses, including high-refractive-index, low-dispersion, and infrared-transmitting materials. These are often utilized in lenses, prisms, and other optical components requiring precision and high performance. With a strong commitment to research and development, SUMITA continually innovates to meet the evolving demands of the optics industry. Their rigorous quality control processes ensure that products meet the highest standards for optical clarity, consistency, and reliability. SUMITA Optical Glass, Inc. has garnered a reputation for excellence and innovation, making it a preferred supplier for organizations in need of advanced optical solutions.