Wavelength: µm
 (0.3–2.4)  
 

Complex refractive index (n+ik)[ i ]


n   k   LogX   LogY   eV

Derived optical constants

Dispersion formula

$$n^2=2.9830277-0.010435952λ^{2}+0.036346467λ^{-2}+0.0026194115λ^{-4}-0.00017513176λ^{-6}+2.1325099\text{×}10^{-05}λ^{-8}$$

Conditions

temperature: 298

Notes

Leaded

References

Data

[Expressions for n]   [CSV - comma separated]   [TXT - tab separated]   [Full database record]

Additional information

Properties of PBH25

thermal_dispersion:
  - 
    type: formula A
    coefficients: 1.331e-05 0.0 0.0 0.0 0.0 0.0
nd: 1.761797
Vd: 27.107724
glass_code: 762271
glass_status: preferred
density:
  - 
    value: 4790
thermal_expansion:
  - 
    temperature_range: 243 343
    value: 7.5E-6
  - 
    temperature_range: 293 573
    value: 8.5E-6
dPgF: 0.0085
resistance:
  acid: 3.2
  phosphate: 2.2

About

Ohara Group is an international group of companies with headquarters in Japan and subsidiaries in Japan (Ohara, Inc.), United States (Ohara Corporation), and Germany (Ohara, GmbH). Ohara is known for its specialization in high-quality optical glass, ceramics, and other advanced materials. With a history spanning over a century, Ohara has been at the forefront of optical innovations, producing a wide range of specialized glass types including low-dispersion and high-refractive-index materials. These are used in various demanding applications like telescopes, microscopes, and high-performance camera lenses. The company's commitment to research and development has led to groundbreaking products such as low thermal expansion glass-ceramics and other specialty materials used in semiconductor manufacturing and space telescopes. With stringent quality control procedures, Ohara ensures that its optical glass meets the highest standards of clarity, consistency, and performance. Their materials are widely regarded for their exceptional quality and are often used in scientific research, aerospace, and other fields where precision and reliability are paramount. Ohara's reputation for technical excellence and innovation makes it a key player in the global optics and materials science industries, providing cutting-edge solutions for a range of complex applications.