Optical constants of MgO:LiNbO3 (Magnesium oxide doped lithium niobate)
Gayer et al. 2008: SLN, 1 mol % MgO; n(e) 0.5–4.0 µm
Wavelength:
µm
(0.5–4)
Complex refractive index (n+ik)
n
k
LogX
LogY
eV
Derived optical constants
Dispersion formula
$$n^2=5.078+\frac{0.0964}{λ^2-0.2065^{2}}+\frac{61.16}{λ^2-10.55^{2}}-1.59\text{×}10^{-2}λ^{2}$$Conditions
temperature: 297.65 optical_component: e
Notes
24.5 °C. Extraordinary optical constants (e). Congruently grown lithium niobate SLN) doped with 1 mol. % MgO. See the original publication for temperature-dependent refractive index equations.
References
O. Gayer, Z. Sacks, E. Galun, A. Arie. Temperature and wavelength dependent refractive index equations for MgO-doped congruent and stoichiometric LiNbO3. Appl. Phys. B 91, 343-348 (2008). Also see Erratum.