Optical constants of HOYA - Optical glass
M-TAF401

Wavelength: µm
 (0.310–1.550)  
 

Complex refractive index (n+ik)[ i ]


n   k   LogX   LogY   eV

Derived optical constants

Dispersion formula

$$n^2=3.07279-0.01366385λ^{2}+0.02527346λ^{-2}+0.000612182λ^{-4}-1.147045\text{×}10^{-05}λ^{-6}+1.543\text{×}10^{-06}λ^{-8}$$

Conditions

temperature: 293

Notes

Glass for molded optics lens

References

Data

[Expressions for n]   [CSV - comma separated]   [TXT - tab separated]   [Full database record]

Additional information

Properties of M-TAF401

thermal_dispersion:
  - 
    type: formula A
    coefficients: 8.39412e-06 0.0 0.0 0.0 0.0 0.0
nd: 1.77377
Vd: 47.17
glass_code: 774472
glass_status: standard
density:
  - 
    value: 4620
thermal_expansion:
  - 
    temperature_range: 243 343
    value: 6.1E-6
  - 
    temperature_range: 293 573
    value: 7.7E-6
dPgF: -0.0078
resistance:
  climatic: "1.0"
  stain: "2.0"
  acid: "3.0"

About

HOYA Corporation is a global technology company based in Japan, known for its diverse range of products in the fields of healthcare and optics. In the optical industry, HOYA is particularly recognized for its high-quality optical glass and lens technologies. The company produces a wide array of optical products, from eyeglass lenses with advanced coatings to specialized glass materials used in cameras, telescopes, and other precision optical instruments. HOYA's expertise extends to various types of optical glass, including low-dispersion and high-refractive-index materials, which find applications in situations requiring exceptional optical clarity and performance. Beyond its contributions to optics, HOYA has also ventured into medical technologies, making it a multi-faceted company with a broad impact. With a commitment to innovation and quality, HOYA has earned a reputation as a leader in its field, consistently delivering products that set industry standards for performance and reliability. Their expansive portfolio and technological prowess make them a go-to provider for both consumer and industrial optical solutions.