RefractiveIndex.INFO

Refractive index database

nk database   |   n2 database   |   raw data + AI   |   about

Shelf

Book

Page

Optical constants of CRYSTRAN - Optical materials
GLS - Gallium lanthanum sulphide

Wavelength: µm
 (0.50–10.60)  
 

Complex refractive index (n+ik)[ i ]


n   k   LogX   LogY   eV

Derived optical constants

Notes

Gallium Lanthanum Sulphide is a radically new chalcogenide glass and a much awaited alternative to toxic Arsenic-based glasses, with an optical transparency from the visible to infrared wavelengths, and thermal stability up to 550oC. In addition, GLS can be melted in a large scale without the need for sealed ampoule processing making GLS production and processing safer and more economical. Equally important, impurity levels, in particular, OH- and SH- absorption bands at around 3 and 4 ìm have been substantially reduced thus increasing performance.
GLS has found use in a wide range of optoelectronic applications and is available as polished optical components, thin and thick films and in optical fibre form.
Gallium Lanthanum Sulphide (GLS) glass is produced by proprietary processes under conditions of the highest purity. Particular effort is made in removing transition metal impurities to a level of better than 1 ppm total metallic impurities with SH- and OH- less than 1 ppm. GLS is routinely processed from ingots of 500 grams. Other glass compositions are available including rare earth doped (Ce, Pr, Nd, Tb, Dy, Ho, Er, Tm, Yb), halide (F, Cl), and Ag doped samples.
REFERENCES:
(1) Petrovich, Hewak et al Journal of Non-Crystalline Solids 326&327 (2003) 93–97°K-1

References

Data

[CSV - comma separated]   [TXT - tab separated]   [Full database record]

Additional information

Properties of GLS - Gallium lanthanum sulphide

density:
  - 
    value: 4040
thermal_dispersion:
  - 
    type: constant
    value: 7.5E-5
thermal_expansion:
  - 
    temperature: 273
    value: 1.0E-5
hardness:
  - 
    type: Knoop
    indenter_mass: 0.2
    value: 2020000000
melting_point:
  - 
    value: 1103
thermal_conductivity:
  - 
    temperature: 273
    value: 0.43
youngs_modulus:
  - 
    value: 59000000000
poissons_ratio:
  - 
    value: 0.24
solubility:
  - 
    value: 0