RefractiveIndex.INFO

Refractive index database

nk database   |   n2 database   |   raw data + AI   |   about

Shelf

Book

Page

Optical constants of CRYSTRAN - Optical materials
CsBr - Caesium bromide

Wavelength: µm
 (0.190–40.000)  
 

Complex refractive index (n+ik)[ i ]


n   k   LogX   LogY   eV

Derived optical constants

Conditions

temperature: 300

Notes

Caesium Bromide is grown by sealed ampoule Stockbarger technique. CsBr is a soft pliable material. IUPAC International Union of Pure and applied Chemistry recommends the spelling as Cesium. UK Useage is Caesium. Solubility has historically been quoted as 124g/100mL at 25°C but Crystran Ltd tests 2021 have found this to be inaccurate.
REFERENCES:
(1) Handbook Optical Constants, ed Palik, V3, ISBN 0-12-544423-0
(2) Mitsuishi et al., J Opt Soc. Am. V52, p14, 1962
(3) Kelly, Bureau of Mines Bulletin, No371, p51, 1934
(4) S.Ballard et al; J.Opt.Soc.Am. Vol42, p684, 1952
(5) H.H.Li; J.Phys. Chem. Ref. Data. Vol 5, No 2. 1976
(6) K.Matthews. Crystran Ltd Test Data 2021

References

Data

[CSV - comma separated]   [TXT - tab separated]   [Full database record]

Additional information

Properties of CsBr - Caesium bromide

density:
  - 
    value: 4400
thermal_dispersion:
  - 
    type: constant
    wavelength: 6.0E-7
    value: 8.4E-5
thermal_expansion:
  - 
    temperature: 273
    value: 4.79E-5
hardness:
  - 
    type: Knoop
    value: 191000000
melting_point:
  - 
    value: 909
thermal_conductivity:
  - 
    temperature: 273
    value: 0.94
youngs_modulus:
  - 
    value: 15850000000
poissons_ratio:
  - 
    value: 0.279
solubility:
  - 
    temperature: 284
    value: 420
  - 
    temperature: 288
    value: 560
  - 
    temperature: 298
    value: 900
  - 
    temperature: 300
    value: 980
  - 
    temperature: 301.5
    value: 1020
  - 
    temperature: 304
    value: 1180
  - 
    temperature: 308
    value: 1380