Optical constants of MgO:LiNbO3 (Magnesium oxide doped lithium niobate)
Gayer et al. 2008: CLN, 5 mol % MgO; n(o) 0.5–1.7 µm
Wavelength:
µm
(0.5–1.7)
Complex refractive index (n+ik)
n
k
LogX
LogY
eV
Derived optical constants
Dispersion formula
$$n^2=5.6533+\frac{0.1185}{λ^2-0.2091^{2}}+\frac{89.61}{λ^2-10.85^{2}}-1.97\text{×}10^{-2}λ^{2}$$Conditions
temperature: 297.65 direction: o
Comments
24.5 °C. Ordinary ray (o). Congruently grown lithium niobate (CLN) doped with 5 mol. % MgO. See the original publication for temperature-dependent refractive index equations.
References
O. Gayer, Z. Sacks, E. Galun, A. Arie. Temperature and wavelength dependent refractive index equations for MgO-doped congruent and stoichiometric LiNbO3. Appl. Phys. B 91, 343-348 (2008). Also see Erratum.