RefractiveIndex.INFO

Refractive index database

nk database   |   n2 database   |   raw data + AI   |   about

Shelf

Book

Page

Optical constants of KTiOPO4 (Potassium titanyl phosphate, KTP)
Kato and Takaoka 2002: n(z) 0.43–3.54 µm

Wavelength: µm
 (0.43–3.54)  
 

Complex refractive index (n+ik)[ i ]


n   k   LogX   LogY   eV

Derived optical constants

Dispersion formula [ i ]

$$n^2=4.59423+\frac{0.06206}{λ^2-0.04763}+\frac{110.80672}{λ^2-86.12171}$$

Conditions

temperature: 293
optical_component: z

Comments

nz; 20 °C.

References

K. Kato and E. Takaoka. Sellmeier and thermo-optic dispersion formulas for KTP. Appl. Opt. 41, 5040-5044 (2002).

Data

[Expressions for n]   [CSV - comma separated]   [TXT - tab separated]   [Full database record]

Additional information

About Potassium titanyl phosphate

Potassium titanyl phosphate (KTiOPO4, commonly abbreviated as KTP) is a nonlinear optical material widely used in a variety of photonic applications, including frequency doubling of laser sources, optical parametric oscillation, and electro-optic modulation. KTP exhibits a broad transparency range from approximately 350 nm to 4.5 μm. One of its noteworthy advantages is its high damage threshold, which makes it suitable for high-power laser applications. The crystal also exhibits good phase-matching conditions over an extensive range of wavelengths, making it a material of choice for tunable and multi-wavelength laser sources. It's commonly utilized in green laser pointers via frequency doubling of Nd:YAG or Nd:YVO4 lasers, which emit at 1064 nm. Overall, KTP's combination of optical and mechanical properties make it an important material in the field of nonlinear optics.