Optical constants of SUMITA - Glasses for precision molding
K-PG375

Wavelength: µm
 (0.365 – 1.548)  
 

Derived optical constants

logX   logY   eV

Dispersion formula

$$n^2=2.3459430-7.7317211\text{×}10^{-3}λ^{2}+1.1783664\text{×}10^{-2}λ^{-2}+2.5239185\text{×}10^{-4}λ^{-4}-1.2352344\text{×}10^{-5}λ^{-6}+8.7540057\text{×}10^{-7}λ^{-8}$$

Comments

Glass for Precision Molding. Refractive index is relative to air at standard conditions; Wavelength in dispersion formula is as measured in air and expressed in micrometers.