Optical constants of SCHOTT - Inquiry glasses
SF6G05

Wavelength: µm
 (0.46 – 2.5)  
 

Derived optical constants

n   k   logX   logY   eV

Dispersion formula [ i ]

$$n^2-1=\frac{1.62113942λ^2}{λ^2-0.0113478992}+\frac{0.506586092λ^2}{λ^2-0.0535840223}+\frac{10.4032298λ^2}{λ^2-1118.83658}$$

Conditions & Spec sheet

n_is_absolute: false
λ_is_vacuum: false
temperature: 20.0 °C
coefficients_of_thermal_dispersion: 6.9e-06 1.76e-08 -3.17e-11 1.89e-06 1.5e-09 0.256
n_d: 1.80906
V_d: 25.28
glass_code: 809253.520
glass_status: special
density: 5.2 g/cm3
coefficient_of_thermal_expansion_1: 7.8e-06 K-1
ΔP_gF: 0.108
climatic_resistance: 4.0
stain_resistance: 3.0
acid_resistance: 51.3
alkali_resistance: 2.3
phosphate_resistance: 3.3

Comments

inquiry glass

References

SCHOTT Zemax catalog 2015-07-22

Data

[Expressions for n]   [CSV - comma separated]   [TXT - tab separated]   [Full database record]

INFO

SCHOTT AG

SCHOTT AG is a German glass manufacturer. SCHOTT also publishes a glass catalog (SCHOTT Optical Glass Datasheets), which is a standard reference for the properties of many optical glasses.

External links


Glass

External links