 (0.29 – 2.4)  
 

Derived optical constants

n   k   logX   logY   eV

Dispersion formula [ i ]

$$n^2-1=\frac{1.26231429λ^2}{λ^2-0.00695586355}+\frac{0.22515421λ^2}{λ^2-0.0221310699}+\frac{0.639119345λ^2}{λ^2-63.1662736}$$

Comments

Improved XMT at 365

Data

[Expressions for n]   [CSV - comma separated]   [TXT - tab separated]   [Full database record]

Additional information

n_is_absolute: false
λ_is_vacuum: false
temperature: 25.0 °C
coefficients_of_thermal_dispersion: 3.6e-06 1.41e-08 -3.59e-11 4.39e-07 5.79e-10 0.167
n_d: 1.589130
V_d: 61.233033
glass_code: 589612
density: 3.23 g/cm3
coefficient_of_thermal_expansion_1: 5.7e-06 K-1
coefficient_of_thermal_expansion_2: 7.2e-06 K-1
ΔP_gF: -0.0026
climatic_resistance: 2.0
acid_resistance: 4.2
phosphate_resistance: 1.0

References

1) OHARA i-line glass data
2) OHARA Zemax catalog 2015-12-01

More info - wiki

Ohara Group is an international group of companies with headquarters in Japan and subsidiaries in Japan (Ohara, Inc.), United States (Ohara Corporation), and Germany (Ohara, GmbH). Ohara manufactures optical and electronic products and also offers measurement services, in particular measurement of refractive indices of solids and liquids.