About chromatic dispersion:
Dispersion (optics) - Wikipedia
Chromatic dispersion of FUSED SILICA at 0.5876 µm:
dn/dλ = -0.0352 µm-1
Dispersion curve:
Dispersion formula:
n2 - 1 = C1λ2/(λ2-C22) + C3λ2/(λ2-C42) + C5λ2/(λ2-C62)
C1 = 0.6961663 C2 = 0.0684043 C3 = 0.4079426 C4 = 0.1162414 C5 = 0.8974794 C6 = 9.896161
Expression for n (C):
sqrt( 1 + 0.6961663*pow(x,2)/(pow(x,2)-pow(0.0684043,2)) + 0.4079426*pow(x,2)/(pow(x,2)-pow(0.1162414,2)) + 0.8974794*pow(x,2)/(pow(x,2)-pow(9.896161,2)) )
Expression for n (FORTRAN):
SQRT( 1 + 0.6961663*x**2/(x**2-0.0684043**2) + 0.4079426*x**2/(x**2-0.1162414**2) + 0.8974794*x**2/(x**2-9.896161**2) )
Expression for n (Visual Basic):
SQR( 1 + 0.6961663*x^2/(x^2-0.0684043^2) + 0.4079426*x^2/(x^2-0.1162414^2) + 0.8974794*x^2/(x^2-9.896161^2) )
Calculated using refractive index data from Refractive index database
|