RefractiveIndex.INFO Refractive index database

Shelf

Book

Page

Optical constants of Mg:LiTaO3 (Magnesium-doped lithium tantalate)
Moutzouris et al. 2011: n(o) 0.450-1.551 µm; 8 mol.% Mg

Wavelength: µm
 (0.45 – 1.551)  
 

Other optical constants

logX   logY   eV

Dispersion formula

$$n^2=4.46828481-0.01791123λ^{2}+0.10437434λ^{-2}-2.84541849\text{×}10^{-3}λ^{-4}+7.87317793\text{×}10^{-4}λ^{-6}$$

Comments

8 mol% Mg-doped congruent lithium tantalate (MCLT). Extraordinary ray(e). 22 °C (see the original publication for temperature-dependent dispersion formula).

Data

[Expressions for n]   [CSV - comma separated]   [TXT - tab separated]   [Full database record]

References

K. Moutzouris, G. Hloupis, I. Stavrakas, D. Triantis and M.-H. Chou. Temperature-dependent visible to near-infrared optical properties of 8 mol% Mg-doped lithium tantalate, Optical Materials Express 1, 458-465 (2011)

More info - wiki

Magnesium-doped lithium tantalate, Mg:LiTaO3

External links