Optical constants of SCHOTT - SSK (Very dense flint)
N-SSK5

Wavelength: µm
 (0.35 – 2.5)  
 

Other optical constants

n   k   logX   logY   eV

Dispersion formula [ i ]

$$n^2-1=\frac{1.59222659λ^2}{λ^2-0.00920284626}+\frac{0.103520774λ^2}{λ^2-0.0423530072}+\frac{1.05174016λ^2}{λ^2-106.927374}$$

Data

[Expressions for n]   [CSV - comma separated]   [TXT - tab separated]   [Full database record]

Additional information

n_is_absolute: false
λ_is_vacuum: false
temperature: 20.0 °C
coefficients_of_thermal_dispersion: 7.29e-07 1.17e-08 -1.5e-11 6.08e-07 7.66e-10 0.189
n_d: 1.65844
V_d: 50.88
glass_code: 658509.371
glass_status: standard
density: 3.71 g/cm3
coefficient_of_thermal_expansion_1: 6.8e-06 K-1
coefficient_of_thermal_expansion_2: 8e-06 K-1
ΔP_gF: -0.0007
climatic_resistance: 2.0
stain_resistance: 3.0
acid_resistance: 52.2
alkali_resistance: 2.2
phosphate_resistance: 3.2

References

1) SCHOTT optical glass data sheets 2015-07-22
2) SCHOTT Zemax catalog 2015-07-22

More info - wiki

SCHOTT AG is a German glass manufacturer. SCHOTT also publishes a glass catalog (SCHOTT Optical Glass Datasheets), which is a standard reference for the properties of many optical glasses.

External links