Optical constants of SCHOTT - SF (Dense flint)
SF4

Wavelength: µm
 (0.365 – 2.5)  
 

Other optical constants

n   k   logX   logY   eV

Dispersion formula [ i ]

$$n^2-1=\frac{1.61957826λ^2}{λ^2-0.0125502104}+\frac{0.339493189λ^2}{λ^2-0.0544559822}+\frac{1.02566931λ^2}{λ^2-117.652222}$$

Comments

lead containing glass type

Data

[Expressions for n]   [CSV - comma separated]   [TXT - tab separated]   [Full database record]

Additional information

n_is_absolute: false
λ_is_vacuum: false
temperature: 20.0 °C
coefficients_of_thermal_dispersion: 5.6e-06 1.7e-08 -5.27e-11 1.54e-06 1.46e-09 0.266
n_d: 1.7552
V_d: 27.58
glass_code: 755276.479
glass_status: standard
density: 4.79 g/cm3
coefficient_of_thermal_expansion_1: 8e-06 K-1
coefficient_of_thermal_expansion_2: 8.9e-06 K-1
ΔP_gF: 0.0062
climatic_resistance: 1.0
stain_resistance: 2.0
acid_resistance: 4.3
alkali_resistance: 2.3
phosphate_resistance: 3.3

References

1) SCHOTT optical glass data sheets 2015-07-22
2) SCHOTT Zemax catalog 2015-07-22

More info - wiki

SCHOTT AG is a German glass manufacturer. SCHOTT also publishes a glass catalog (SCHOTT Optical Glass Datasheets), which is a standard reference for the properties of many optical glasses.

External links