Optical constants of SCHOTT - SF (Dense flint)
SF11

Wavelength: µm
 (0.39 – 2.5)  
 

Other optical constants

n   k   logX   logY   eV

Dispersion formula [ i ]

$$n^2-1=\frac{1.73848403λ^2}{λ^2-0.0136068604}+\frac{0.311168974λ^2}{λ^2-0.0615960463}+\frac{1.17490871λ^2}{λ^2-121.922711}$$

Comments

lead containing

Data

[Expressions for n]   [CSV - comma separated]   [TXT - tab separated]   [Full database record]

Additional information

n_is_absolute: false
λ_is_vacuum: false
temperature: 20.0 °C
coefficients_of_thermal_dispersion: 1.12e-05 1.81e-08 -5.03e-11 1.46e-06 1.58e-09 0.282
n_d: 1.78472
V_d: 25.76
glass_code: 785258.474
glass_status: standard
density: 4.74 g/cm3
coefficient_of_thermal_expansion_1: 6.1e-06 K-1
coefficient_of_thermal_expansion_2: 6.8e-06 K-1
ΔP_gF: 0.0142
climatic_resistance: 1.0
stain_resistance: 0.0
acid_resistance: 1.0
alkali_resistance: 1.2
phosphate_resistance: 1.0

References

1) SCHOTT optical glass data sheets 2015-07-22
2) SCHOTT Zemax catalog 2015-07-22

More info - wiki

SCHOTT AG is a German glass manufacturer. SCHOTT also publishes a glass catalog (SCHOTT Optical Glass Datasheets), which is a standard reference for the properties of many optical glasses.