RefractiveIndex.INFO Refractive index database

Shelf

Book

Page

Optical constants of SCHOTT - SF (Dense flint)
N-SF57

Wavelength: µm
 (0.37 – 2.5)  
 

Other optical constants

n   k   logX   logY   eV

Dispersion formula [ i ]

$$n^2-1=\frac{1.87543831λ^2}{λ^2-0.0141749518}+\frac{0.37375749λ^2}{λ^2-0.0640509927}+\frac{2.30001797λ^2}{λ^2-177.389795}$$

Data

[Expressions for n]   [CSV - comma separated]   [TXT - tab separated]   [Full database record]

Additional information

n_is_absolute: false
λ_is_vacuum: false
temperature: 20.0 °C
coefficients_of_thermal_dispersion: -4.51e-06 8.73e-09 -1.64e-11 1.07e-06 1.57e-09 0.295
n_d: 1.84666
V_d: 23.78
glass_code: 847238.353
glass_status: standard
density: 3.533 g/cm3
coefficient_of_thermal_expansion_1: 8.46e-06 K-1
coefficient_of_thermal_expansion_2: 9.88e-06 K-1
ΔP_gF: 0.0178
climatic_resistance: 1.0
stain_resistance: 0.0
acid_resistance: 1.0
alkali_resistance: 1.0
phosphate_resistance: 1.0

References

1) SCHOTT optical glass data sheets 2015-07-22
2) SCHOTT Zemax catalog 2015-07-22

More info - wiki

SCHOTT AG is a German glass manufacturer. SCHOTT also publishes a glass catalog (SCHOTT Optical Glass Datasheets), which is a standard reference for the properties of many optical glasses.

External links