RefractiveIndex.INFO Refractive index database

Shelf

Book

Page

Optical constants of SCHOTT - SF (Dense flint)
N-SF14

Wavelength: µm
 (0.365 – 2.5)  
 

Other optical constants

n   k   logX   logY   eV

Dispersion formula [ i ]

$$n^2-1=\frac{1.69022361λ^2}{λ^2-0.0130512113}+\frac{0.288870052λ^2}{λ^2-0.061369188}+\frac{1.7045187λ^2}{λ^2-149.517689}$$

Data

[Expressions for n]   [CSV - comma separated]   [TXT - tab separated]   [Full database record]

Additional information

n_is_absolute: false
λ_is_vacuum: false
temperature: 20.0 °C
coefficients_of_thermal_dispersion: -5.56e-06 7.09e-09 -1.09e-11 9.85e-07 1.39e-09 0.287
n_d: 1.76182
V_d: 26.53
glass_code: 762265.312
glass_status: standard
density: 3.118 g/cm3
coefficient_of_thermal_expansion_1: 9.41e-06 K-1
coefficient_of_thermal_expansion_2: 1.087e-05 K-1
ΔP_gF: 0.013
climatic_resistance: 1.0
stain_resistance: 0.0
acid_resistance: 1.0
alkali_resistance: 1.0
phosphate_resistance: 1.0

References

1) SCHOTT optical glass data sheets 2015-07-22
2) SCHOTT Zemax catalog 2015-07-22

More info - wiki

SCHOTT AG is a German glass manufacturer. SCHOTT also publishes a glass catalog (SCHOTT Optical Glass Datasheets), which is a standard reference for the properties of many optical glasses.

External links