Optical constants of SCHOTT - LaSF (Lanthanum dense flint)
N-LASF46A

Wavelength: µm
 (0.37 – 2.5)  
 

Other optical constants

n   k   logX   logY   eV

Dispersion formula [ i ]

$$n^2-1=\frac{2.16701566λ^2}{λ^2-0.0123595524}+\frac{0.319812761λ^2}{λ^2-0.0560610282}+\frac{1.66004486λ^2}{λ^2-107.047718}$$

Data

[Expressions for n]   [CSV - comma separated]   [TXT - tab separated]   [Full database record]

Additional information

n_is_absolute: false
λ_is_vacuum: false
temperature: 20.0 °C
coefficients_of_thermal_dispersion: 3.53e-06 1.24e-08 -1.87e-11 8.39e-07 1.04e-09 0.275
n_d: 1.90366
V_d: 31.32
glass_code: 904313.445
glass_status: standard
density: 4.449 g/cm3
coefficient_of_thermal_expansion_1: 6e-06 K-1
coefficient_of_thermal_expansion_2: 7.15e-06 K-1
ΔP_gF: 0.0042
climatic_resistance: 1.0
stain_resistance: 0.0
acid_resistance: 3.0
alkali_resistance: 1.0
phosphate_resistance: 1.0

References

1) SCHOTT optical glass data sheets 2015-07-22